316L vs. Titanium vs. Hastelloy C276: Choosing Sintered Filter Alloy by Medium
Four alloys cover most sintered filter duty. The choice is decided by three things - chloride, temperature and whether the environment is oxidizing or reducing.
Most filter failures we are asked to explain are not sintering failures. They are alloy-selection failures: the right part in the wrong metal, failing in months instead of years. This article sets out how the four common sintered filter alloys divide the work, using the three variables that actually decide it.
The three questions that decide the alloy
- Is there chloride? Chloride is the single most common cause of pitting and stress corrosion cracking in stainless steel. Trace chloride plus warmth plus oxygen is enough.
- What temperature? Above roughly 400-500 °C the choice narrows quickly, and above 800 °C only a few alloys remain practical.
- Is the environment oxidizing or reducing? Sulphuric acid, hydrochloric acid and many process streams are reducing; nitric acid and many bleaches are oxidizing. An alloy that excels in one can fail quickly in the other.
The four alloys in practice
| Alloy | Strong in | Fails in | Typical duty |
|---|---|---|---|
| 316L | Water, steam, food and beverage, pharmaceutical, dilute organic acids, moderate chloride at low temperature | Chloride pitting above ~60 °C, strong reducing acids, high-temperature sulphidation | Most general filtration; the default when nothing exotic is present |
| Titanium (TA1 / ASTM Gr. 1-2) | Seawater, chlorinated water, oxidizing acids, hypochlorite, excellent strength-to-weight, good at moderate-high temperature | Reducing acids (HCl, H2SO4 at strength), dry chlorine, methanol, fluoride | Desalination, marine, chlor-alkali, chemical processes with oxidizers |
| Hastelloy C276 | Wet chlorine, hypochlorite, ferric and cupric chlorides, sulphuric and hydrochloric acid across concentrations, mixed acid streams | Strong oxidizing media (use C22 or a different family), and it is expensive - not a default | Chemical processing, flue gas, pickling lines, pharmaceutical intermediates |
| Inconel 600 / 625 | High temperature to about 1000-1100 °C, oxidation resistance, carburising atmospheres, some chloride at high temperature | Aqueous chloride service (not its strength), reducing acid service | Furnace atmospheres, hot gas filtration, syngas, heat treating |
How the decision usually goes
Step 1 - no chloride, moderate temperature: 316L. It is the cheapest and, for water, steam, food and most pharmaceutical duty, entirely adequate. Do not upgrade "for safety" without a reason: a finer alloy often has worse machining behaviour and higher cost without solving anything.
Step 2 - chloride present: titanium if the environment is oxidizing and the temperature is moderate; C276 if the environment is reducing, or if the chloride concentration and temperature are both high. Seawater is the classic titanium case; wet chlorine and hypochlorite are the classic C276 case.
Step 3 - high temperature: Inconel 600 or 625, with the choice depending on whether the atmosphere is oxidizing or carburising. Above 1100 °C, sintered metal filters are generally outside their practical range regardless of alloy.
Step 4 - mixed or unknown: describe the actual stream rather than picking an alloy. A stream that is "dilute acid with some chloride at 80 °C" can eliminate 316L and titanium both, and the answer is usually C276 or C22.
The three selection mistakes we see most
- 316L in warm chloride. Cooling water with 200 ppm chloride at 70 °C will pit 316L. Titanium or a super-austenitic grade is the fix; more frequent replacement is not.
- Titanium in reducing acid. Titanium's passive film needs oxygen. In strong HCl or H2SO4 without an oxidizer, it corrodes fast - faster than 316L in some cases.
- C276 as a default "best" alloy. C276 is excellent, and expensive. Using it where 316L would last ten years spends money on nothing.
Relative cost, so you can plan
As a rough order for the same geometry: 304 is the base, 316L is modestly above it, titanium is several times the stainless price, and C276 is higher again. Exact ratios move with mill prices, but the ranking is stable. This is why the material question should be answered by the medium, not by habit.
What to send us
Medium (composition if known), chloride level, pH, working temperature, pressure, and whether the stream is oxidizing or reducing. With those five items we can usually name the alloy on the first reply - and tell you if the answer is "316L is enough", which happens more often than suppliers admit.
Questions we get asked
- Can 316L be used in seawater?
- Not reliably. Chloride pitting and crevice corrosion attack 316L in seawater even at ambient temperature. Titanium, or a super-austenitic/duplex grade where strength demands it, is the usual answer.
- Is titanium always better than stainless?
- No. Titanium is excellent in oxidizing chloride environments and poor in reducing acids. In plain water or steam it adds cost without benefit.
- What is the maximum temperature for a sintered metal filter?
- For Inconel 600/625, about 1000-1100 °C in suitable atmospheres. Stainless grades are practical to roughly 400-500 °C depending on atmosphere; titanium is limited by oxidation above about 400 °C in air.
- Can you supply a material certificate with the alloy?
- Yes - certificate of material with heat/lot number and composition accompanies every batch, and third-party verification is available from a CNAS-accredited laboratory.
Describe the medium, chloride level, pH and temperature. We will answer with a recommendation - including "316L is enough" when it is. [email protected]